性能项目 | 试验条件[状态] | 测试方法 | 测试数据 |
密度 | | ASTMD1505 | 0.916 | g/cm3 |
熔流率(熔体流动速率)(190°C/2.16kg) | | ASTMD1238 | 1.4 | g/10min |
薄膜厚度-经测试 | | | 25 | um |
割线模量-1%正割,MD(25um) | | ASTMD882 | 172 | MPa |
SecantModulus-1%Secant,TD(25um) | | ASTMD882 | 190 | MPa |
TensileStrength-MD(Yield,25um) | | ASTMD882 | 13.1 | MPa |
TensileStrength-TD(Yield,25um) | | ASTMD882 | 9.93 | MPa |
TensileStrength-MD(Break,25um) | | ASTMD882 | 52.7 | MPa |
TensileStrength-TD(Break,25um) | | ASTMD882 | 46.9 | MPa |
伸长率-MD(断裂,25um) | | ASTMD882 | 480 | % |
TensileElongation-TD(Break,25um) | | ASTMD882 | 600 | % |
DartDropImpact3(25um) | | ASTMD1709 | 800 | g |
埃尔曼多夫抗撕强度-MD(25um) | | ASTMD1922 | 230 | g |
ElmendorfTearStrength-TD(25um) | | ASTMD1922 | 500 | g |
光泽度(60°,25.4um,吹塑薄膜) | | ASTMD2457 | 93 | |
雾度(25.4um,吹塑薄膜) | | ASTMD1003 | 11 | % |